新闻资讯

新闻资讯

current position: Home > News Center > Industry Information

Anhydrous neodymium chloride manufacturers share research progress in the preparation and application of cerium dioxide nanomaterials (Part 2)

2022-06-21 13:20:27
times

(Continued)


After the SCR catalyst is used for a long time, the denitration performance will gradually decline until the catalyst performance can not meet the NOx control requirements. Catalyst regeneration technology is to use cleaning, loading and other processes to restore the activity of the catalyst so as to extend the service life of the catalyst. SCR catalyst regeneration technology has high economic and environmental value. The modification of mercury oxidizing substances in the catalyst regeneration process can improve the regeneration level, save the purchase cost of new catalysts, and increase the mercury oxidation capacity of catalysts, which has a broad application prospect.


However, the technology of combining SCR catalyst regeneration and mercury oxidation modification is rarely reported. In this study, deactivated catalysts of domestic power plants are selected as the research objects, and CeO2 modification technology and catalyst regeneration technology are combined to improve the HGO oxidation performance of SCR catalysts on the basis of restoring their original physical and chemical properties, which has high economic and practical value.


2. oxidation characteristics of elemental mercury of CeO 2 modified regenerated SCR catalyst

2.1 materials and samples


The deactivated honeycomb SCR catalyst of a 1000 MW coal-fired power unit in China was used as the object to study the modification and regeneration of CeO2. The catalyst monomer is 20 × 20 holes, size 150mm × 150mm × 1250mm, which has been used for more than 40000 hours by the time of sampling. Sodium hydroxide (NaOH), concentrated sulfuric acid (H2SO4), vanadium oxysulfate (VOSO4) and cerium nitrate (CE (NO3) 3 · 6H2O) used for catalyst regeneration are commercial reagents and analytically pure.


2.2 CeO2 modification and regeneration method


In this study, the process of "cleaning + loading + calcination" was adopted to modify and regenerate the deactivated SCR catalyst.


The deactivated SCR catalyst monomer used in the experiment was cut to form 6 × 6-hole catalyst sample block with size of 50mm × 50mm × 50mm。 Immerse the sample block in deionized water for water washing for 1h, take it out and wash it in 0.015% hydrofluoric acid for 1H. After the first step of pickling is completed, wash it in o 1mol / L H2SO4 solution for 30min, supplemented by ultrasonic disturbance. And then placed in clean water for rinsing for 1H. Thus, the cleaning process of the deactivated catalyst is completed.


Prepare a VOSO4 solution with a mass fraction of 1.5% as the loading solution. Weigh a certain amount of Ce (NO3) 3 · 6H2O, put it into 300ml of loading solution, stir evenly and fully dissolve it, and then put it into the cleaned catalyst sample block. After fully loading LOMIN, take out the catalyst sample block, put it in the oven, dry it at 95 ℃ for 1h, take it out, and calcine it at 600 ℃ for 4H to prepare CeO2 modified regenerated catalyst sample.


In this study, deactivated SCR catalyst, ordinary regenerated SCR catalyst and CeO2 modified regenerated SCR catalyst were used to study the oxidation of elemental mercury. The deactivated catalyst is named cat, the ordinary regenerated sample is named recat, and the CeO2 modified regenerated sample is named xcerecat (where X represents the mass percentage of CeO2 in the sample, x = 0.5, 1.0, 3.0, 5.0). After crushing and grinding, all samples were sieved through 40-60 mesh, and the prepared granular samples were tested for mercury oxidation performance in a self-made fixed bed reactor.


2.3 mercury oxidation performance test of samples


The self-made fixed bed reaction system is shown in Fig. 1. The simulated flue gas is composed of no, NH3, SO2, O2, H2O, HGO and N2. Wherein H2O comes from the steam generator; The HGO comes from the HGO generating device composed of a mercury permeation tube and a thermostatic water bath, and is brought into the simulated flue gas by the carrier gas N2; Other components are from cylinder gas, and the flow is controlled by mass flowmeter.


Fig. 1 Schematic diagram of Hg0 oxidation test device

The components of flue gas enter the self-made fixed bed reactor after passing through the mixer. The reactor is made of a quartz tube with a diameter of 8mm, and is externally heated and insulated by a heat tracing belt. The test sample is placed in the constant temperature section of the reactor. The concentration of HGO in flue gas was measured by vm-3000 mercury analyzer (mercury instruments, Germany). The flue gas at the outlet of the reactor is discharged after being treated by the activated carbon tail gas treatment system. Each part of the system is connected by silica gel flue gas pipeline, and the part containing HGO and H2O is traced by tracing belt to prevent condensation. The tracing temperature is 150 ℃. The temperature of heat tracing pipeline and reactor in the system is controlled by K-type thermocouple.


2.4 HGO oxidation performance of CeO2 modified regenerated catalyst


In order to explore the oxidation ability of different samples to HGO, the "50 μ g/m3 HgO+4%O2+15 μ L / L HCl + balanced N2 "as the basic flue gas condition, the mercury oxidation efficiency of the deactivated catalyst, the ordinary regenerated catalyst and the CeO2 modified regenerated catalyst was tested at 280 ~ 380 ° C. The experimental results are shown in Fig. 2. The deactivated catalyst cat has very low HGO oxidation capacity at various temperature points, and the upper limit HGO oxidation efficiency of cat is only 51.2% at 340 ℃. After ordinary regeneration (without CeO2 modification), the HGO oxidation efficiency of the sample was significantly improved. The oxidation performance of recat was very high at 340 ℃, and the HGO oxidation efficiency was 69.3%. Combined with the bet and XRF analysis of the sample, the surface impurities of the catalyst were cleaned after regeneration treatment, and the original active sites and pore structures were re exposed, which greatly improved the oxidation performance of the catalyst. In addition, the V loading process effectively added surfactant, making the oxidation of HGO more obvious.

 

Fig. 2 HGO oxidation efficiency of sample

CeO2 modification significantly improved the oxidation performance of HGO. As shown in Fig. 2, the mass fraction of CeO2 in the 0.5 cerecat sample is only 0.5%, and its HGO oxidation efficiency has reached 75.3% at 320 ℃, and the lower limit of HGO oxidation efficiency is 62.5% at 280 ℃. It shows that the addition of CE has a strong promoting effect on the surface oxidation ability of the catalyst.


After CeO2 modification, the Ce3 + / Ce4 + redox electric pair on the catalyst surface can provide a large amount of active oxygen for the oxidation process of HGO, thus promoting the oxidation ability of the sample HGO. The HGO oxidation ability of the sample was further enhanced by increasing the CeO2 loading. 3. The HGO oxidation efficiency of O cerecat sample at 300 ~ 320 ℃ is about 91.7%, which is the highest among all samples.


After further increasing the CeO2 loading, the HGO oxidation efficiency of 5. O cerecat sample at the experimental temperature is slightly lower than that of 3. O cerecat. When the loading is excessively increased, the active components will accumulate on the surface of the catalyst, resulting in pore structure blockage, thus inhibiting the oxidation of HGO by the sample. In addition, when the flue gas temperature of CeO2 modified regenerated sample in Fig. 2 is greater than 320 ℃, the HGO oxidation efficiency decreases with the continuous increase of flue gas temperature. On the one hand, a higher flue gas temperature will inhibit the adsorption of HGO in the flue gas on the catalyst surface, thereby inhibiting the combination of HGO and active oxygen on the catalyst surface, resulting in a decrease in the oxidation efficiency of HGO; On the other hand, when the flue gas temperature rises, part of the oxidized mercury will be decomposed again to form HGO.


2.5 conclusion

(1) The CeO2 modified regeneration method can effectively clean the deactivated SCR catalyst, remove the surface impurities and recover the surface active sites and pore structure after regeneration; The addition of CE during the loading process will not have a negative impact on the original loading process, and the process of loading CE and V can effectively improve the physical and chemical characteristics of the catalyst surface.

(2) The regenerated catalyst modified by CeO2 has excellent oxidation performance of HGO. The upper limit HGO oxidation efficiency of 3. O cerecat is 91.7%, and it has good anti SO2 and anti H2O characteristics. When CeO2 modified regeneration catalyst is placed in the lower layer of SCR system, the NH3 content in flue gas is low, and the oxidation effect of HGO is good, which has application prospects.

(3) Using deactivated SCR catalyst for CeO2 modification and regeneration can effectively improve the HGO oxidation performance of the catalyst and achieve the purpose of resource reuse, which has good application value and environmental protection significance.




Main references

(1) Zhang Peng, et al., progress in the preparation of nano cerium dioxide and its photocatalytic performance, modern chemical industry, online launch date: 2020-08

(2) He Chuan, et al., oxidation characteristics of elemental mercury of CeO2 modified regenerated SCR catalyst, modern chemical industry, online launch date: 2020-07

(3) Li Lin, et al., effect of nano CeO2 on the aging resistance of RTV silicone rubber coatings, rare earth: 2020 (1)



Tags

Related news

  • menu